Machine × material · Settings
OMTech 60W settings for 3 mm cast acrylic
OMTech's 60W chart says 15 mm/s optimal at 95% for 3 mm acrylic. Their blog says 10–15 mm/s at 65–75% for a 60–80W CO2.
- Machine
- OMTech MF1624-60, a 60W CO2
- Material
- Cast acrylic, and how it differs from extruded
- Rows
- 4
Settings on this page
| Job | Laser | Power | Speed | Passes | Interval | Focus | Where it came from |
|---|---|---|---|---|---|---|---|
| Cut | CO2 | 95% (the chart note) | 15 mm/s optimal, 20 mm/s maximum | not stated | not stated | not stated | Cited |
| Cut | CO2 | 65–75% | 10–15 mm/s | not stated on this row | not stated | about halfway through the thickness | Cited |
| Engrave | CO2 | 15–30% | 400–750 mm/s | single pass, as printed | 300–500 DPI, as printed | not stated | Cited |
| Cut | CO2 | 80% max, 70% min | 10 in the file, read here as 10 mm/s | not set in the file | not set in the file | not set in the file | Starting estimate The file stores speed 10 with no unit, max power 80, and min power 70, for acrylic-clear at thickness 3. The same file's plywood cut is the one this site reads as mm/s. The author says the numbers are for their machines. The entry says clear acrylic, not cast, and it does not name the MF1624-60. |
This is 3 mm acrylic, about 1/8 inch, on the MF1624-60. Cast versus extruded is explained on the acrylic page. Leave the masking on. The cabinet listing is the machine, not a material kit.
What each row is
The chart’s 60W acrylic line for 3 mm is 20 mm/s maximum and 15 mm/s optimal, and the chart note says laser power is 95%. The same note says to keep face air modest, or blow from the side, so the edge stays smooth, and to keep air under the sheet so it does not burn. Passes and focus are not in that cell.
The blog’s 60W to 80W cut row is 10–15 mm/s at 65–75%. A nearby sentence gives a 40–50W baseline “in a single pass.” That pass count is not copied onto the 60–80W row, because the article did not put it there. Focus, in the acrylic tips, is about halfway through the sheet. The article also says not to live at 100% power. The chart’s 95% and the blog’s 65–75% are both OMTech. They are not averaged here.
The engrave row is the blog’s general CO2 band: 15–30% power, 400–750 mm/s, 300–500 DPI, one pass. It is not labeled 60W only. On a 60W tube, start the test at 15% and the fast end of that speed. Cast acrylic is the one they say turns frosty white. Turn the air down for the engrave or the frost can look cloudy.
The LightBurn row is acrylic-clear at thickness 3 in omt-60w.clb: speed 10, minimum power 70, maximum power 80. The unit note is in the table. “Clear” is not the same word as “cast.”
Run a test grid first
Cut a square out of a masked scrap from the same sheet. Honeycomb or a blade bed, so the back does not bounce the beam. For a cut test, power 60% to 80% and speed 8 to 18 mm/s covers the blog row. Add a single square at the chart’s 15 mm/s and a high power only if you want to see that row, and watch for flame.
If the edge chars
Acrylic usually melts more than it chars, but a yellow, sooty, or flamed edge is the same problem: too much heat, or not enough air under the sheet. Speed up inside the blog range before you climb toward 95%. If the edge is gummy, OMTech’s own distinction may be the reason: extruded sheet does that. Cast is the better cut.
If it does not cut through
The square stays hinged at the bottom. Drop toward 10 mm/s before you add a second pass. Confirm the focus is in the middle of the sheet, not on the masking. A 1/4 inch sheet is not this row. The chart’s 5 mm optimal cell is 7 mm/s at the same 95% note, and this page is not a 5 mm page. Do not type the 3 mm speed and hope.
What would change the number
Color, cast versus extruded, a weak compressor, and a tired tube. Clear acrylic on the F1’s diode is a different machine. xTool does not promise clear acrylic to that diode. Do not bring this CO2 table to a diode.
Questions people ask
Which cut row should I type in first?
Start the scrap test inside the blog's 65–75% band, around 10 mm/s. That corner is inside a range OMTech printed for a 60–80W CO2. The 95% chart is also theirs. It is the harder row, and it is the one to open only if the lower row does not cut through.
Will extruded acrylic use the same cut?
OMTech says extruded acrylic cuts and is more likely to melt, with a gummy edge. The cut range can be a starting test. The frosty engrave they describe is for cast. If the engrave looks clear or grey, you probably have extruded sheet.
Sources
- OMTech laser cutting recommended parameters — OMTech
- Material settings for laser engravers — OMTech
- LightBurn library omt-60w.clb — clvLabs
- OMTech Maker MF1624-60 product page — OMTech